Every number a design engineer needs on one page — with the test conditions attached, because a strength figure without a method is marketing.
Silicon nitride (Si₃N₄) sits in an unusual position among engineering ceramics: it is tough enough to be used as a rolling element, hard enough to cut cast iron, thermally stable enough to survive a 1,000 °C quench, and electrically insulating enough to sit inside a power module. No other single material covers that range. The cost of that range is that its properties are process-dependent — a gas-pressure sintered grade and a HIP grade of the same nominal composition differ by 30–40% in strength and by more in reliability.
This page is the reference we send when a customer asks "what are your properties". It gives typical values with test conditions, explains which grade to specify for which application, and lists the data you should demand from any supplier before you approve a drawing.
| Property | GPS grade | HIP grade | Hot-pressed (HP) | Test condition |
|---|---|---|---|---|
| Density | 3.20–3.25 g/cm³ | 3.22–3.26 g/cm³ | 3.22–3.28 g/cm³ | Archimedes, > 99% theoretical |
| Flexural strength | 700–900 MPa | 900–1,100 MPa | 900–1,200 MPa | 4-point bend, RT, 3 × 4 × 40 mm |
| Weibull modulus m | 8–12 | 15–25 | 10–18 | 4-point bend, ≥ 20 specimens |
| Fracture toughness KIC | 6.0–7.5 MPa·m0.5 | 7.0–9.0 MPa·m0.5 | 5.5–7.0 MPa·m0.5 | SEVNB or single-edge notched beam |
| Vickers hardness | 1,400–1,550 HV | 1,450–1,600 HV | 1,500–1,700 HV | HV1, 9.8 N, 15 s |
| Elastic modulus | 300–310 GPa | 305–320 GPa | 310–320 GPa | Resonant beam / ultrasonic |
| Poisson's ratio | 0.26–0.28 | 0.26–0.28 | 0.26–0.28 | Resonant beam |
| Compressive strength | 2,500–3,000 MPa | 3,000–3,500 MPa | 2,800–3,500 MPa | Uniaxial, RT |
| Tensile strength (direct) | 400–500 MPa | 500–650 MPa | 450–600 MPa | Button-head specimen, RT |
| Fracture surface energy | 25–40 J/m² | 30–45 J/m² | 25–40 J/m² | Derived from KIC and E |
Two relationships in that table do most of the engineering work. Compression is roughly six times tension — which is why ceramic parts are designed to be preloaded, shrink-fitted or seated, never hung in bending. And toughness of 6–9 MPa·m0.5 is what separates silicon nitride from alumina (3–4 MPa·m0.5): it is the reason a Si₃N₄ bearing ball can survive a fatigue load that would spall alumina, and the reason it tolerates the edge chips and handling abuse that would start a crack in a less tough ceramic.
| Property | Typical value | Note / condition |
|---|---|---|
| Coefficient of thermal expansion | 3.0–3.4 ×10⁻⁶/K | RT–1,000 °C; about one third of steel, one quarter of aluminium |
| Thermal conductivity | 20–30 W/m·K | Structural grades, RT. High-conductivity substrate grades reach 80–90 W/m·K |
| Specific heat capacity | 700–800 J/kg·K | RT |
| Thermal diffusivity | 8–11 mm²/s | Structural grades |
| Max continuous service temperature | 1,000 °C | Oxidising atmosphere; short excursions to 1,200 °C |
| Max temperature, inert atmosphere | 1,350–1,400 °C | Limited by grain-boundary phase, not by the Si₃N₄ grains |
| Critical quench ΔT (water) | 500–700 °C | No cracking in a single water quench from temperature |
| Softening / creep onset | ~1,100–1,200 °C | Grade-dependent; HIP grades with cleaner grain boundaries hold longer |
The combination of low expansion and high strength is what makes silicon nitride the default for thermal-cycling duty: welding nozzles, riser tubes, thermocouple sheaths, heat-treatment fixtures. Its thermal shock resistance comes not from low conductivity (which is mediocre) but from a high strength-to-modulus ratio. Where the application needs conductivity as well — power-module substrates — a dedicated substrate grade is required, and that is a different product line from a structural grade.
| Property | Typical value | Condition |
|---|---|---|
| Volume resistivity | > 10¹³ Ω·cm | RT |
| Dielectric constant εr | 7.5–8.5 | 1 MHz, RT |
| Dielectric loss (tan δ) | 1–3 ×10⁻⁴ | 1 MHz, RT |
| Dielectric strength | 15–20 kV/mm | AC, 1 mm specimen, in oil |
| Breakdown voltage (0.32 mm substrate) | > 5 kV | Substrate grade, > 10 kV/mm |
Silicon nitride is an insulator in structural service and a dielectric in RF and power service. For power modules the relevant figure is not the bulk dielectric strength but the partial-discharge resistance under repeated thermal cycling, where Si₃N₄ outperforms both Al₂O₃ and AlN because its mechanical toughness resists the micro-cracking that initiates PD in a ceramic substrate. That is the whole argument for Si₃N₄ AMB substrates in EV traction inverters.
| Medium | Resistance | Practical note |
|---|---|---|
| Mineral acids (HCl, H₂SO₄, HNO₃) — dilute to moderate | Good to excellent | Standard grade is fine up to moderate concentration and temperature |
| Hydrofluoric acid (HF) | Poor | Attacks both the Si₃N₄ and the grain-boundary phase. Do not specify Si₃N₄ for HF service |
| Hot concentrated phosphoric acid | Poor | Dissolves the intergranular glass; use alumina or SiC instead |
| Hot concentrated NaOH / KOH (> 100 °C) | Poor | The classic trap in alumina refineries. SSiC or a non-oxide alternative is the correct choice |
| Molten aluminium | Good | Not wetted by aluminium; the standard material for riser tubes, rotors and sheaths |
| Molten salts, slags | Variable | Fluoride-bearing melts attack the grain boundary; test with a coupon first |
| Oxidation in air above 1,000 °C | Gradual | Forms a protective SiO₂ layer; growth is parabolic, but it consumes material over thousands of hours |
| Water / steam, static fatigue | Susceptible | Slow crack growth under sustained tensile stress in humid conditions — use HIP plus proof testing for critical parts |
The pattern worth memorising: silicon nitride is a good material for acids and molten metals, and a bad one for HF, hot phosphoric acid, and hot concentrated alkali. Two of the three failures we get asked to analyse in chemical service are one of those three media, not a manufacturing defect.
Silicon nitride is not one material. The three production routes give three property profiles, and choosing the wrong one is the most common and most expensive specification mistake.
| Grade route | What it is | Strength / Weibull | Shape capability | Specify it for |
|---|---|---|---|---|
| Gas-pressure sintered (GPS) | Densified at 1,750–1,900 °C under 1–10 MPa nitrogen, so the material does not decompose | 700–900 MPa / m 8–12 | Complex shapes, near-net forming, economical | Wear parts, seal rings, riser tubes, thermocouple sheaths, general structural parts |
| GPS + HIP | Gas-pressure sintered, then hot-isostatically pressed at 1,700–2,000 °C / 100–200 MPa | 900–1,100 MPa / m 15–25 | Same shapes, higher cost, near-zero internal porosity | Bearing balls, probe-card guides, pump plungers, valve components, anything where one flaw ends the part's life |
| Hot-pressed (HP) | Uniaxial pressing at 1,700–1,800 °C in graphite dies | 900–1,200 MPa / m 10–18 | Simple plates, blocks, discs — no complex 3D shapes | Cutting-tool blanks, substrate blanks, armour tiles, fine-grain plates |
| Substrate grade | Tape-cast, sintered, < 1 mm, controlled thermal conductivity and surface finish | — | Flat sheets 0.25–1.0 mm | AMB / DBC substrates for SiC and IGBT power modules |
| Application | Grade | Why this grade | Typical spec to agree |
|---|---|---|---|
| Bearing balls (hybrid / full ceramic) | HIP | Rolling contact fatigue is flaw-initiated; m > 15 and proof testing decide life | G5–G10 grade, ΔD ≤ 0.13 µm, Ra ≤ 0.02 µm |
| Seal rings and valve seats | GPS or HIP | Flatness and thermal stability matter more than peak strength | Flatness 0.6–0.9 µm, Ra 0.05–0.1 µm on the face |
| LPDC riser tubes | GPS | Thermal cycling plus molten aluminium; toughness prevents crack growth at the metal line | Wall 5–10 mm, no through-wall porosity, 1,000+ cycles |
| Thermocouple sheaths, heater tubes | GPS | Thermal shock and chemical inertness, closed-end geometry | Gas-tight to 1 × 10⁻⁸ Pa·m³/s, wall 2–5 mm |
| Probe card guides and plates | HIP, fine grain | Sub-micron hole arrays and long service without particle shedding | Hole ±2 µm, flatness 2 µm, Ra ≤ 0.1 µm |
| Pump plungers, valve balls | HIP | Proof testing truncates the weak tail; downtime cost is high | Roundness 0.5 µm, Ra 0.05 µm, proof tested to 1.5× service stress |
| Cutting tool blanks | HP or Sialon | Fine grain for edge sharpness; hot pressing makes plates efficiently | Grain < 1 µm, edge chipping < 20 µm |
| AMB substrates | Substrate | Need partial-discharge resistance and thermal cycling, not bulk strength | 0.25–0.635 mm, Ra 0.2–0.4 µm, camber < 3 µm/10 mm |
Properties are only half a specification; the other half is what the factory can actually hold. Typical capability on our line:
| Feature | Capability | Note |
|---|---|---|
| Forming routes | Dry pressing, cold isostatic pressing, tape casting, injection moulding | CIP for large or high-uniformity parts; tape casting for substrates |
| Sintering | 15 GPS furnaces, 9 HIP furnaces, 3 hot presses | Route selected per part, not per batch convenience |
| Diameter / length | Up to ~300 mm (CIP), larger on review | Larger parts change the strength calculation via stressed volume |
| General tolerance | ±0.01 mm ground | ±0.005 mm achievable on selected features |
| Surface roughness | Ra 0.1–0.4 µm ground; 0.02–0.05 µm polished | Tensile surfaces should be specified explicitly |
| Flatness | 1–2 µm on 50 mm faces | Lapping; matters for seals and substrates |
| Holes | Ø0.3 mm and up; ±5 µm on precision arrays | Diamond drilling and ultrasonic machining |
| Threads | Internal and external, M3 and up | Thread roots are stress raisers — expect a design discussion |
If a quotation arrives with a single strength number and no test conditions, it is not a specification. Ask for:
NitriCeram runs a dedicated silicon nitride line in Zibo, Shandong: powder synthesis, forming, sintering and diamond grinding under one roof. We operate 15 gas-pressure sintering furnaces, 9 hot-isostatic pressing furnaces and 3 hot-press furnaces, with 2 Si₃N₄ substrate lines. A ~100-person R&D team (15 PhDs, 40+ MSc) runs in-house density, phase, microstructure, strength, thermal and reliability testing under an ISO 9001 system, and we proof test parts to an agreed stress on request.
Send the drawing and the operating conditions — temperature, load, cycles, medium — and we will tell you which grade the duty actually requires, and where a cheaper grade would do just as well.
Typical four-point bend strength at room temperature is 700–900 MPa for a gas-pressure sintered grade, 900–1,100 MPa for a HIP grade, and 900–1,200 MPa for hot-pressed fine-grain material. Those figures are averages over test bars; the design value must account for the Weibull modulus and the stressed volume of the actual part. A single number without test conditions should not be used for design.
In flexural strength, silicon nitride (700–1,100 MPa) is comparable to or better than zirconia (800–1,000 MPa) and roughly double alumina (300–400 MPa). The bigger difference is fracture toughness: 6–9 MPa·m^0.5 for Si₃N₄ against 3–5 for zirconia and 3–4 for alumina. Toughness, not strength, is what determines tolerance to impacts, edge chips and rolling-contact fatigue.
About 1,000 °C continuous in air, with short excursions to roughly 1,200 °C. In an inert atmosphere it can go to 1,350–1,400 °C. The limit is set by the grain-boundary glassy phase, which softens and oxidises, not by the silicon nitride grains themselves — which is why cleaner HIP grades hold their strength to a higher temperature than standard GPS grades.
No. HF attacks both the nitride and the intergranular phase, and hot concentrated NaOH or KOH dissolves the grain-boundary glass. The same applies to hot concentrated phosphoric acid. For those media, alumina or silicon carbide is the correct family, and often the choice is between them rather than silicon nitride.
Three reasons: silicon nitride powder is far more expensive than alumina powder; sintering requires gas-pressure furnaces at 1,750–1,900 °C rather than air furnaces at 1,500 °C; and diamond grinding is slow because the material is hard and, unlike alumina, does not respond to cheap finishing routes. HIP adds a second high-pressure furnace cycle. The premium buys toughness and thermal shock resistance that alumina cannot provide at any price.
Specify GPS for general wear parts, seal rings, riser tubes and sheaths, where moderate strength and a Weibull modulus of 8–12 are enough. Specify HIP when a single flaw would end the part's life — bearing balls, probe-card guides, pump plungers, valve components — because HIP removes internal porosity and raises both strength and the reliability that comes with a high Weibull modulus. HIP roughly adds a second sintering cycle to the cost.
See our silicon nitride parts → GPS vs HIP sintering → Why parts fail → Ask an engineer →